24 IdentIfyIng PaInt defects SOlVENT pOp Description Open blisters on the finished surface causes • Too much air flow over repair area • Solvent trapped in the film during the curing process forming bubbles in the paint film • High film builds • Using too fast of a reducer and/or hardener for the spray conditions • Bake temperature too high or IR lamp too close to the surface prevention • Use appropriate reducer and/or hardener for spray booth conditions per product data sheets • Apply recommended film builds per product data sheet • Keep booth at recommended bake temperature and times • Insure proper spray booth air flow correcting • Sand surface blisters smooths and refinish • Severe cases must be sanded back to undercoat and refinished