5 IdentIfyIng PaInt defects BlISTERING Description Small bubbles or pimples ranging in size from .5mm - 1.5mm in the topcoat application causes • High humidity • Improper surface cleaning • Incompatibility of materials • Excessive film builds • Water, oil, or dirt in airlines prevention • Insure you are within recommended film build per product data sheet • Select proper reducer for spray conditions • Carefully clean substrate • Do not touch cleaned areas with bare hands • Drain and clean compressor and regulator to remove trapped contaminants correcting • Establish where the blisters are • If in between layers, sand blisters down to a solid surface and refinish • In severe cases the finish will need to be removed and refinished